The work presents an analysis of the recycling potential of thin-walled aluminum within the framework of a circular economy (CE). The analysis focused on the undersized fraction derived from the processing of municipal waste in Mechanical Biological Treatment (MBT) facilities. After the mechanical processing of the incoming waste, it passes through screens, where the so-called undersized fraction is separated, the composition of which varies over time due to the seasonality of municipal waste and the origin of the waste. As part of the conducted work, an attempt was made to determine the variability over time; the studies lasted 12 months and assessed the possibility of recovering thin-walled aluminum from the municipal waste stream. During the research, a series of trial melts were performed using modified fluxes based on cryolite with the addition of NaCl. The work was carried out using a laboratory induction crucible furnace
The growing demand for manufacturing steel components in the manufacturing industry is forcing the rapid development of metal welding technology. One of the modern welding techniques is the joining of components using laser welding, where the material is joined using a focused laser beam. This method makes it possible to achieve high process efficiency, while maintaining cleanliness in the welding area and high-quality welded joints. In the conducted research, the laser beam welding method (method 52) was compared with the conventional TIG welding method (method 141), to compare the welding time, the effect of temperature in the HAZ after welding and the quality of the resulting welds.
This publication presents the results of dielectric strength tests conducted on selected materials. The methodology for sample fabrication is described, utilizing two different spatial printing technologies. The tested samples were manufactured from four materials with varying properties: PLA, ABS, PA12, and a recycled material (e-PLA). Significant differences in dielectric strength were observed, both among the individual materials and between the applied manufacturing technologies. It was determined that samples made of PA12, produced using laser sintering (SLS) technology, exhibited the highest dielectric strength. The objective of the study was to evaluate the feasibility of producing insulating components for power transmission and distribution lines through dielectric strength testing. Preliminary results indicate that, with the appropriate technology and material selection, this manufacturing approach may be a viable alternative for such applications.
The study presents a series of experiments focused on cleaning the active surface of a conventional grinding wheel using two methods of supplying the cooling and lubricating fluid with minimum consumption: MQL (Minimum Quantity Lubrication) and the flood method WET (wet machining) with an oil–water emulsion, during the process of plunge surface grinding in both up- and down-grinding modes. The tests were carried out on steel grade 1.4034 with a hardness of 55 HRC. A special design solution of the 38A60KV8 grinding wheel (Norton Poland) was proposed, which enabled observation of the behavior and deposition of contaminants on the sample surface. A methodology was developed for collecting contaminants on the surface of the ground material. The contaminants from the active surface of the grinding wheel (CPS) were weighed. The obtained results made it possible to assess the effectiveness of the investigated methods of supplying the cooling and lubricating fluid (PCS). In particular, it was found that perpendicular delivery of PCS supports the lubrication of the ground surface, positively affects the cutting forces by reducing friction, and consequently lowers the temperature in the machining zone, which in turn contributes to achieving a more favorable distribution of compressive stresses in the surface layer.”
This paper presents an analysis of the anisotropy of mechanical properties of the investigated sheets based on the results of static tensile testing and HV hardness measurements. The objective of the study was to evaluate variations in mechanical properties in three key areas along the coil length. In addition, an analysis across the sheet width was performed. It was found, among other things, that there are clear differences in hardness between the beginning, middle, and end areas of the coil. The differences in hardness ranged from approximately 2.3 to as much as 12.9 units, with higher values observed for hot-rolled sheets. Differences in hardness between the edge and the center of the sheet were also observed in all three zones. The largest differences in yield strength and tensile strength values, regardless of steel grade, were obtained across the sheet width at the beginning or end of the coil. Based on the analysis of the obtained results, the level of anisotropy of the mechanical properties of the sheets was determined for the individual dimensions and steel grades. The results demonstrated that anisotropy is more pronounced across the sheet width than along the coil length. It was also shown that hot-rolled sheets exhibit higher anisotropy compared to cold-rolled sheets. The obtained results provided the basis for developing an innovative tension-straightening technology for sheets uncoiled from coils and formed into flat sheets.
Praca została dofinansowana ze środków Narodowego Centrum Badań i Rozwoju (NCBiR), nr grantu POIR.01.01.01-00-0477/18.
This study numerically investigates the ballistic behavior of stitched and unstitched carbon fiber-reinforced composite plates using the finite element method. Simulations were performed under high-velocity impact conditions using ANSYS Workbench, with a projectile velocity of 350 m/s and appropriate boundary constraints. The results reveal that stitched composites exhibit higher values in internal (4.90 × 10⁵ J) and contact energy components (5.56 × 10⁵ J) compared to unstitched composites (4.22 × 10⁵ J and 1.19 × 10⁵ J, respectively). This indicates that stitching enhances load transfer at the fiber–matrix interfaces and facilitates more effective distribution of the absorbed energy through structural deformation. Although unstitched composites show slightly higher total energy absorption (5.74 × 10⁶ J) than stitched ones (5.52 × 10⁶ J), a significant portion of this energy remains in the form of kinetic energy (5.32 × 10⁶ J vs. 5.27 × 10⁶ J), contributing less to structural absorption. Consequently, while unstitched composites demonstrate a more brittle behavior, stitched composites dissipate energy more effectively through internal deformation and contact mechanisms, resulting in superior ballistic performance. The findings provide valuable insights for the design of impact-resistant composite structures in defense and aerospace applications.
The paper characterizes the castings of bottom plates used in chamber furnaces for heat treatment. Their typical structures and damages that occur in these castings during operation are presented. Bottom plates usually have a rectangular shape adapted in dimensions to the hearth of chamber furnaces. They consist of one or several segments, depending on the length of the furnace chamber. They are cast in sand molds. Plate castings are commonly made of high-chromium heat-resistant cast steel or heat-resistant chromium-nickel cast steel melted in crucible induction furnaces. Appropriate grades of cast steel and operating conditions of plates in which the use of individual alloys is recommended are indicated. Material, design and casting factors that plate designers take into account to ensure appropriate functional properties of castings are also discussed. This work is a review, its main purpose being to provide a summary of the current state of knowledge and the most important issues related to the design, manufacture, and operation of bottom plates.
This paper presents a comparative analysis of tool steels applied in cutting forms for paper cutlery manufacturing. The study was initiated after the original tool material, martensitic stainless steel 440C (HRC 56–58), demonstrated insufficient wear resistance plus is easily damaged, broken and required frequent sharpening. Four alternative Uddeholm steels—Sverker 21, Sleipner, Unimax, and Tyrax ESR—were tested under identical production conditions. Two of them (Unimax and Sverker 21) were coated with Duplex-Tigral PVD coating. The objective was to evaluate wear mechanisms, lifetime, and maintenance needs during stamping of 1000 gsm laminated cupstock paper. Tool wear was assessed using visual inspection and 3D scanning after approximately 500,000 cutting cycles. The results revealed that coated Unimax and Sleipner steels offered improved durability and reduced adhesive wear compared to the baseline. Average sharpening intervals increased from 0.5 to nearly 1 million cycles, although below the designed 2 million. Premature wear and paper residue accumulation caused additional downtime of up to 10 days per sharpening. The study highlights that an optimal combination of tool steel grade and PVD coating can significantly reduce maintenance frequency and operational costs in automated paper cutlery production.
The main purpose of this paper is the presentation of possibilities of using elements of SPC in the analysis of selected parameters of product manufactured in an industrial enterprise producing metal components and the analysis of causes of parameter deviations in control charts and their correction possibilities. As a tested product metal element used in automotive industry was chosen. Five parameters of the manufactured product were tested. During production process every hour 6-element samples were taken. In the analysis 30 samples were considered. Statistical analysis of selected parameters was done. According to this analysis the causes of parameter deviations in control charts were identified and their correction possibilities were proposed. As main causes of problems three main types of elements were identified: machines, tools and people.
Traceability is essential in modern manufacturing to ensure product quality, safety, and compliance throughout production and operation. In sectors such as automotive and aerospace, reliable component identification supports process control, maintenance, and failure analysis. Conventional marking methods often fail under difficult thermal conditions, creating demand for more robust solutions. This study evaluates the durability and readability of laser-engraved codes on aluminum components under conditions representative of industrial environments. Codes were engraved on surfaces with varying geometries, textures, and temperature, then exposed to elevated temperatures treatments. Their performance was assessed using industrial and mobile scanning devices to determine suitability for traceability systems in demanding manufacturing processes.
Comparative Analysis of Steel Cutting Forms Used for Paper Cutlery Production
- 1. Department Department of Materials Engineering and Production Systems (K14), Faculty of Mechanical Engineering, Lodz University of Technology (Politechnika Lodzka),
Abstrakt
This paper presents a comparative analysis of tool steels applied in cutting forms for paper cutlery manufacturing. The study was initiated after the original tool material, martensitic stainless steel 440C (HRC 56–58), demonstrated insufficient wear resistance plus is easily damaged, broken and required frequent sharpening. Four alternative Uddeholm steels—Sverker 21, Sleipner, Unimax, and Tyrax ESR—were tested under identical production conditions. Two of them (Unimax and Sverker 21) were coated with Duplex-Tigral PVD coating. The objective was to evaluate wear mechanisms, lifetime, and maintenance needs during stamping of 1000 gsm laminated cupstock paper. Tool wear was assessed using visual inspection and 3D scanning after approximately 500,000 cutting cycles. The results revealed that coated Unimax and Sleipner steels offered improved durability and reduced adhesive wear compared to the baseline. Average sharpening intervals increased from 0.5 to nearly 1 million cycles, although below the designed 2 million. Premature wear and paper residue accumulation caused additional downtime of up to 10 days per sharpening. The study highlights that an optimal combination of tool steel grade and PVD coating can significantly reduce maintenance frequency and operational costs in automated paper cutlery production.
Introduction
Growing demand for sustainable and biodegradable food packaging has accelerated the development of paper-based cutlery as an alternative to single-use plastics. In large-scale production, cutting forms play a critical role in maintaining dimensional accuracy and surface quality of the final products. The original machine setup used 440C stainless steel cutting forms (HRC 56–58), which demonstrated premature wear and frequent need for regrinding. This negatively affected production continuity and increased operational costs. To overcome these limitations, four high-performance Uddeholm steels – Sverker 21, Sleipner, Unimax, and Tyrax ESR – were tested under real production conditions to assess their wear resistance and suitability for stamping 1000 gsm laminated paperboard.
Machining, forming, and stamping processes impose increasingly high demands on the durability and reliability of tools. Under intensive operating conditions, tools are exposed to repeated impact loading, micro-vibrations, and fibre-induced abrasion. As a result, steels with insufficient impact toughness tend to develop micro-chipping and crack propagation along the cutting edge. This behaviour was particularly evident in the original 440C tools.
Higher impact toughness correlates with lower susceptibility to micro-chipping and brittle edge failure. Unimax and Sleipner demonstrated significantly higher toughness than 440C and Sverker 21, which explains the observed differences in service life.
Tool damage may occur due to mechanical, thermal, chemical, or tribological factors. The most common failure modes include fatigue cracking, edge chipping, plastic deformation, abrasive and adhesive wear, oxidation, and thermal erosion. The nature and intensity of these processes depend on the type of material being processed, the operating conditions, the tool geometry, and – most importantly – the properties of the material from which the tool is made.
In industrial practice, a wide range of tool materials is used, depending on the specific application. Cold-work tool steels (e.g., X153CrMoV12, D2) and hot-work tool steels (e.g., X40CrMoV5-1, H13) are commonly applied due to their high hardness, wear resistance, and dimensional stability. For more demanding conditions, high-speed steels (HSS) such as HS6-5-2 (M2) or HS10-4-3-10 (M42) offer an excellent balance between hardness and temper resistance. When extremely high mechanical or thermal loads are expected, cemented carbides (WC-Co), cermets, cubic boron nitride (CBN), or technical ceramics are preferred for their superior hardness and temperature stability.
A significant improvement in tool performance can be achieved through the application of thin protective coatings deposited by Physical Vapor Deposition (PVD) methods. Coatings such as TiN, TiAlN, CrN, AlTiN, or multilayer systems like TiAlSiN exhibit high hardness (often exceeding 2000 HV), low friction coefficients, and excellent oxidation resistance at elevated temperatures. The choice of coating depends on the intended operating environment: TiN is suitable for machining carbon and alloy steels, TiAlN performs well under high-temperature conditions, while CrN provides good corrosion resistance and low friction when processing non-ferrous materials such as aluminium or polymers. In recent years, gradient and nanocomposite coatings have gained attention for their ability to combine the benefits of multiple materials and reduce delamination risks.
In summary, tool durability and reliability result from a complex interplay between the tool material, working conditions, and surface phenomena at the tool–workpiece interface. Proper selection of tool steel, microstructural characteristics, and PVD coating type is crucial to minimizing tool damage and significantly extending tool life.
The aim of this work is to select suitable materials for tools used in the industrial production of disposable cutlery, based on preliminary tests of wear, corrosion, and other factors.
Materials and Methods
The tests were conducted under industrial production conditions. The cutting forms were tested in a stamping process for paper forks, knives, and spoons, operating at a cycle time of approximately 1.5 seconds. The cutting dies were made of steel grade: 1.2379/X153CrMoV12, in accordance with ISO 4957:2004. The chemical composition of the X153CrMoV12 alloy is shown in Table 1. Table 2 presents the composition of the previously used cutting material, steel 440C (UNS S44004). Tables 3–6 contain the chemical compositions of the alternative tool steels evaluated as cutting materials in the study: Tyrax ESR, Sleipner, Unimax, and Sverker. Figure 1 presents the approximate Charpy impact toughness of the tool steels [1] included in the analysis.
Table 1. The chemical composition of X153CrMoV12 (1.2379) steel.
Table 2. The chemical composition of steel 440 C, according to the standard UNS S44004.
Table 3. The chemical composition of “Tyrax” from UDDEHOLM.
Table 4. The chemical composition of “Sleipner” from UDDEHOLM.
Table 5. The chemical composition of “Unimax” from UDDEHOLM.
Table 6. The chemical composition of “Sverker” AISI D2, W.-Nr. 1.2379 from UDDEHOLM.
Figure 1. Approximate Charpy Impact Toughness of Tool Steels [1].
All steels were heat-treated according to the manufacturer’s recommendations. Unimax and Sverker 21 were coated with a Duplex-Tigral PVD coating (AlCrTiN-based) to enhance surface hardness and oxidation resistance. Wear was evaluated by visual inspection and 3D scanning after every 500,000 cycles. The assumed tool lifetime was 2,000,000 cycles, while the actual performance was significantly lower.
Results and Discussion
Figures 2–11 show examples of tool wear, chipping, and paper residue accumulation observed during testing. One of the forms was equipped with an insert. These inserts were produced from different materials and tested on the machine during a real life production process. Further tribological tests are planned in the laboratory, using special cubes made from the same material and coatings as the inserts tested in the machine during production. The results will be obtained and compared to the findings of the inserts tests.
In Figure 2, examples of cutting-edge wear and micro-chipping are shown; Figure 3 shows adhesive wear near the fork geometry; Figure 4 presents the Tyrax ESR insert after testing; in Figure 5, a representative image of tool testing in the cutting form is shown; Figure 6 shows a representative image of the tools used in the testing in the cutting form [5]; in Figure 7, there is representative tool damage; Figures 8 and 9 show paper residue accumulation; in Figure 10, the 3-D scanning model used for wear analysis is shown; and in Figure 11, a sample of a paper cutlery fork produced with damaged tooling is shown[10].
Figure 2. Representative image of cutting-edge wear after ~500,000 cycles, showing micro-chipping and radius rounding [1].
Figure 3. Detail of adhesive wear on cutting edges near fork geometry [2].
Figure 4. Tyrax ESR insert after testing, exhibiting plastic deformation at the blade tip [3].
Figure 5. Representative image of tool testing in the cutting form [4].
Figure 6. Representative image of tools used in the testing in the cutting form [5].
Figure 7. Representative image of tool damage [6].
Figure 8. Representative image of paper residue accumulation [7].
Figure 9. Representative image of paper residue accumulation [8].
Figure 10. 3-D scanning model [9].
Figure 11. Sample of paper cutlery fork produced with damaged tooling [10].
The analysis of production data confirmed that steels with lower Charpy impact energy (440C, Sverker 21) exhibited frequent edge chipping and required earlier sharpening. Steels with higher toughness (Unimax, Sleipner) showed primarily uniform abrasive wear with minimal fracture-related damage.
The performance comparison revealed clear differences in tool life and wear mechanisms among the tested steels. Unimax and Sleipner exhibited the highest resistance to chipping and adhesive wear. Tyrax ESR showed good toughness but was prone to edge deformation. Even when coated, Sverker 21 experienced localized chipping and needed resharpening after around 600,000 cycles. Paper residue adhesion was found to accelerate abrasive wear and increase cutting force. The PVD coating improved surface smoothness and delayed oxidation effects, but excessive fibre buildup between tool edges led to dimensional inaccuracies. Cleaning downtime reached approximately 12 days per year, while sharpening cycles caused 7–10 days of machine stop per occurrence. It was observed that humidity and temperature of the surroundings of the machine could impact performance. Additionally, paper humidity has a critical impact on the process. While paper humidity range was established and incorporated into the production process through quality checks and controls during the raw material production process, the lack of control over atmospheric parameters in the production hall, such as temperature and air humidity, will be future areas that the company needs to address.
Conclusions
The research results presented above lead to the following conclusions:
1. The original 440C tool steel was inadequate for continuous paper cutlery production due to insufficient wear resistance.
2. Among the tested materials, Unimax with PVD coating and Sleipner demonstrated the best performance balance between wear resistance and toughness.
3. PVD Duplex-Tigral coating effectively reduced adhesive wear and extended tool life, although regular cleaning remains necessary to prevent fibre accumulation.
4. Optimized maintenance scheduling and selection of tool material can reduce total downtime by up to 30% annually.
5. Hybrid coatings, thermochemical treatments, and controlled-environment operation (humidity, temperature) are recommended as future research directions.
6. Cleaning-related downtime currently reaches ~12 days per year; sharpening causes an additional 7–10 days of machine stop.
7. Environmental parameters in the production hall, particularly humidity and temperature, significantly influence tool wear and process repeatability.
8. Planned tribological tests using dedicated test cubes are expected to quantify the wear behaviour of each steel-coating combination.