Journal of Engineering 360

E-ISSN: 3071-7507
Journal of Engineering 360
JoE360
Published: 30-11-2024
Number of articles: 9
Other articles from this issue
22-10-2024 - Review article
Aneta Jakubus

The paper analyzes and discusses the orientations of researchers regarding the abrasive wear of vermicular cast iron. The analysis was related to the shape of graphite occurrence in cast iron, the change in the matrix and the change in chemical composition, and the impact of these changes on wear under dry and wet friction conditions. Compact graphite cast iron is tested for use in machine and device parts such as cylinders and piston rings, discs, shafts and bearings. It was found that the improvement of abrasive wear of vermicular cast iron is influenced, among others, by the shape of graphite, the alloy addition in the form of tin, as well as the change of the matrix in vermicular cast iron to an ausferritic one. Summarizing the analysis of research carried out by a number of authors, it would be necessary to continue research on the abrasion resistance of this material, and it would also be advisable to include issues related to the warping and deformation of samples as a result of heating and cooling of cast iron.

22-10-2024 - Original article
Dariusz Rydz, Grzegorz Stradomski, Michał Pałęga

This work presents a comparative analysis of the technological process before and after its modernization. The aim of the work was a comparative analysis based on the assessment of the OEE total effectiveness indicator on the example of one of the metal industry companies. The research conducted in this work took into account both the company's technical capabilities and issues related to technological process management. The work contains the characteristics of defined problems and the scope of corrective actions aimed at reducing or completely eliminating them.

22-10-2024 - Original article
Ewa Ociepa, Agata Dudek

The purpose of work was a scientific analysis of lenticular implant intraocular applied in ophthalmology. Lenses of the Alcon Laboratories company were used for surveys. Spectrophotometric, macroscopic and roentgenographic examinations were conducted. The aim of the study was to determine as much information as possible about the analyzed implants using engineering and research methods. The evaluation was carried out as part of an engineering diploma thesis. As a result of the obtained research results, it was found that the applied techniques allow for the correct evaluation of the tested materials.

22-10-2024 - Review article
Anna Fajdek-Bieda, Agnieszka Wróblewska

The review article presents a comprehensive analysis of recent research on biocomposites based on natural minerals as fillers. The various minerals available on the market and their potential to modify and improve the properties of composites are discussed. Methods of manufacturing biocomposites, such as blending, impregnation and coating application, are described in detail, taking into account the importance of process parameters and component ratios for achieving optimal material properties. The article also examines recent scientific developments related to the use of minerals in biocomposites, paying particular attention to their effects on strength, stiffness, environmental resistance and biodegradation. Despite advances in biocomposite manufacturing technology, there is a need for further research into optimizing manufacturing processes to obtain materials with homogeneous properties. Future research should focus on analyzing the effects of different types of minerals and their proportions on the properties of biocomposites. Biocomposites with natural minerals are widely used in various industrial sectors, from construction to automotive and food packaging, suggesting their potential as an alternative to traditional plastics, contributing to the development of greener materials.

30-11-2024 - Original article
Mariola Spalik

The article presents an analysis of the influence of aluminum (Al) and silicon (Si) coating additions on the process of high-temperature oxidation of steel. After high-temperature oxidation of coatings deposited on steel substrates, the oxidation was carried out in an air atmosphere at 800°C for 20 hours. The samples were oxidized on one side, i.e. they were placed on a quartz plate during the test. After oxidation, the unit mass increase of the samples was measured using a laboratory scale with an accuracy of 0.00001 g. It was examined how the addition of these elements affects the formation of protective oxide layers that limit corrosion at elevated temperatures. Aluminum contributes to the formation of stable aluminum oxide (Al₂O₃) layers, while silicon supports the formation of silicon oxide (SiO₂). Both oxides act as protective barriers, reducing the penetration of oxygen into the material, which slows down its degradation. The appropriate concentration of these admixtures improves the steel's resistance to oxidation without significantly impairing its mechanical properties. The article emphasizes the importance of appropriate selection of Al and Si content to increase the durability of steel in high-temperature operating conditions.

30-11-2024 - Original article
Robert Barski

This article presents the possibility of using the magnetic measurement method, which is an alternative method to shearography as a method of testing the condition of the cord of all-steel tires in order to determine the possibility of using the casing for the retreading process. It is an extension of the design and research work aimed at creating a prototype of a diagnostic device. As part of the activities, a prototype of the device and a version of the measuring head were developed, but a prototype of the algorithm of the measurement program was also created, which uses the physical foundations of non-destructive measurements of motor vehicle tires developed within the project. This study is related to the increasingly strict regulations and the intentions of the European Commission regarding the use of vehicles, which require an increase in the share of recycled materials, including tires. Therefore, there is a need to develop measurement methods that allow for the assessment of the quality of the casing while the used tires are still stored. This work presents the results of theoretical analyses of the possibility of using the magnetic field as a diagnostic parameter of the condition of tires

30-11-2024 - Original article
Gernot Wilhelm Rueppel, Oliver Niklas Dorn, Felix Kuke, Lars Ulke-Winter, Holger Seidlitz

Wet-winding is used to manufacture rotationally symmetrical components such as pipes and pressure vessels, as well as non-rotationally symmetrical components like T-connectors. During this process, a resin-impregnated fiber (e.g., glass or carbon fiber) is wound around a core. The winding pattern influences the mechanical properties, including stiffness and strength of the component, and is optimized based on the expected loads. In practice, however, factors such as tape tension and resin content can cause deviations from the predefined winding pattern. This paper proposes a measuring system utilizing an IR-camera to record the winding pattern during production. The collected data is processed and converted into a digital twin for further analysis.

30-11-2024 - Original article
Łukasz Lemieszewski, Dina Hannebauer, Grzegorz Remiszewski

Wi-Fi networks are often susceptible to signal interference that can disrupt services, intercept sensitive data, and allow unauthorized access. Exploiting this vulnerability, attackers can launch Intentional Electromagnetic Interference (IEMI) attacks or protocol-based attacks. IEMI attacks include, but are not limited to, jamming, which involves the introduction of interference signals in the frequency band used by a given Wi-Fi network, thus disrupting its proper operation. The article presents research on different types of IEMI attacks, aimed at illustrating this type of threat to video transmission from Wi-Fi cameras and discusses methods of protection against this type of attack. The paper examines the methods of jamming the wireless network band, which are used on the distribution methods and the Sweeping Jammer methods that cyclically disrupt all available devices. Based on the experiments, it has been confirmed that SOHO devices are highly susceptible to this type of simple attacks and implementing a method to minimize the effects of jamming yields poor results. The simplicity of this type of attack and the high availability of software and hardware tools on the market make the threat highly popular and still dangerous.

30-11-2024 - Original article
Paweł Zmorkowski

The article presents the impact of bearing housing clearance on the operation of a gear transmission, the consequences of operating the equipment under improper technical conditions, and the resulting implications. The article also describes vibration diagnostic methods as a tool for supporting the assessment of the technical condition and identifying the root causes of defects.

 
30-11-2024-Original article - Pages: 46 - 57

Optical tape detection using an IR camera to create a digital twin of rotationally symmetrical wet-wound FRP components

  • 1. Fraunhofer IAP, Department of Polymeric Materials and Composites PYCO
  • 2. BTU Cottbus-Senftenberg, Department of Polymer-Based Lightweight Design
  • 3. BTU Cottbus-Senftenberg,, Department of Polymer-Based Lightweight Design
  • 4. Fraunhofer IAP, Department of Polymeric Materials and Composites PYCO, BTU Cottbus-Senftenberg, Department of Polymer-Based Lightweight Design
Sent to editorial office:08-07-2024
Accepted after review:03-10-2024
Published:30-11-2024

Language versions:
3
42
DOI:10.5604/01.3001.0054.8851
GICID:01.3001.0054.8851


 

Abstrakt

Wet-winding is used to manufacture rotationally symmetrical components such as pipes and pressure vessels, as well as non-rotationally symmetrical components like T-connectors. During this process, a resin-impregnated fiber (e.g., glass or carbon fiber) is wound around a core. The winding pattern influences the mechanical properties, including stiffness and strength of the component, and is optimized based on the expected loads. In practice, however, factors such as tape tension and resin content can cause deviations from the predefined winding pattern. This paper proposes a measuring system utilizing an IR-camera to record the winding pattern during production. The collected data is processed and converted into a digital twin for further analysis.

 

Introduction

The significance of advanced manufacturing processes and lightweight construction materials, such as fiber-reinforced plastics (FRP), is increasing due to the “Sustainable Development Strategy” implemented by the German government in July 2023 [1]. This strategy aims to reduce greenhouse gas emissions and the consumption of primary raw materials. Wet winding, one of the key manufacturing processes for producing lightweight components, is utilized to produce rotationally symmetrical FRP components such as drive shafts, pipes, and pressure tanks as well as non-rotationally symmetrical components like T-connectors. These components offer weight savings of up to 75% when compared to their metallic counterparts [2]. In the wet winding process (see Fig. 1), rovings, which are continuous strands of fibers, are unwound from a spool, Typically, carbon or glass fibers are used as the fiber material. Each fiber spool is placed on an electronically controlled unwinding unit that applies torque opposite to the unwinding direction to maintain specific yarn tension during unwinding. The fibers then pass through a heated resin bath, where they are impregnated with epoxy resin, for example. Once impregnated, the fiber strands are brought together side by side at the delivery eye to form a single tape. This tape is then wound in predetermined patterns over a rotating core or mandrel.

A software application (e.g., Winding Expert by MIKROSAM) is typically used to create winding patterns. Each pattern can be customized by setting parameters such as mandrel geometry, expected tape width, and fiber angle. The software calculates the necessary winding paths to cover the mandrel with fiber material and generates a G-code that can be executed by the winding machine. Winding patterns can essentially be categorized into two types based on the winding angle (φ), as shown in Fig. 2. The first type, called hoop or circumferential winding, involves winding the tape side by side onto the mandrel at an angle of ≈90° to the axis of rotation. This angle depends on the magnitude of the mandrel-radius (R = 55 mm) and the tape width (w) [8].

undefined
Alternate image: Figure 1. Wet winding process. ...

Figure 1. Wet winding process.

The second type is helical winding, which involves winding angles less than 90°. To cover the mandrel, the delivery eye moves back and forth multiple times, causing the fiber tapes to cross each other. Consequently, the winding pattern consists of two angles which are equal in magnitude but opposite in sign. For instance, drive shafts are wound at angles of approximately +-45° to efficiently counteract torsional load.

Alternate image: Figure 2. Different winding patterns. ...

Figure 2. Different winding patterns.

After the winding process, the component undergoes a curing stage, which can take place either at room temperature or in an oven. During this stage, the component is constantly rotated to ensure uniform resin distribution.

The number and sequence of the winding patterns, along with their winding angles and the number of intersections, are typically determined prior to manufacturing through a numerical process aimed at optimizing weight while complying the for strength and rigidity specifications [9]. However, during the actual manufacturing process, factors such as tape tension, resin content and viscosity can lead to variations in the tape’s width and position compared to the simulated winding pattern. These variations may result in incorrect winding angles, gaps, and overlaps, negatively impacting the mechanical properties of the final product [10]. For example, to compensate for these imperfections, pressure vessels need to withstand a minimum burst pressure of at least 225% of the nominal working pressure to be authorized for use in the automotive sector, or even 350% if the vessel is primarily manufactured from glass-fiber [3].

To facilitate quality control in the winding process and to better understand the relationship between process parameters and their impact on the actual winding pattern, this study presents an optical monitoring system based on an infra-red (IR) camera. The monitoring system can reconstruct the winding patterns and generate a digital replica of the laminate structure for further analysis. The choice of thermography as the measuring principle is justified by the temperature difference between the incoming tape, which is warm from the resin, and the previously placed and cooled material. As shown in Fig. 3, the incoming fiber tape is clearly visible in the IR-image as it is wound onto the cylindrical mandrel under investigation in this study.

Alternate image: Figure 3. Camera position and IR-image. ...

Figure 3. Camera position and IR-image.

The main objective is to create a clear distinction between the newly placed material and the previously laid material, enabling an algorithm to identify the edges of the tape and, consequently, its width, position, and angle. Previous research has demonstrated that the contrast in an infra-red image can be enhanced by lowering winding speeds, increasing resin temperature, and applying appropriate gamma correction to the IR-image. This method was successfully tested for hoop winding at speeds up to 0.96m/s [4]. Nevertheless, when using a similar strategy for winding helical patterns, the contrast between intersecting tapes at the turning zones of the mandrel seem insufficient for the edge detection algorithm to accurately detect the correct edges of the tape. Therefore, this study presents an alternative method.

 

Experiment

A 4-axis wet winding machine from Mikrosam, model A.D. MAW 20 LS4/1 (see Fig. 5), is utilized for the winding procedure. This first experiment is limited to cylindrical winding cores. Thus, a thermoplastic tubing with a diameter of 110 mm serves as the mandrel. An IR-camera of the VarioCAM HDx 645 type from InfraTec is mounted on the same carriage as the delivery eye. This makes it possible for the camera to follow the delivery eye during the winding process and capture thermal images of the incoming tape (see Fig. 4). The position of the carriage or camera can be retained from the winding machine via the Beckhoff communication protocol TwinCAT 3 | ADS. The camera operates at a 30 Hz framerate with 640x480 pixel resolution. It looks straight down and is positioned in such a way that the center pixel row of the camera image is aligned with the axis of the mandrel. The area where the tape first comes into contact with the mandrel is slightly below the center row of the camera.

Alternate image: Figure 4. Camera alignment and tape contact. ...

Figure 4. Camera alignment and tape contact.

It should be noted that previous research has shown that, depending on the resin load and tape tension, the width of the tape can increase up to a 90° offset from its initial contact point with the mandrel [5]. To maintain a straightforward test setup, this was not considered in the current study.

Four spools of Tenax-E HTS40 E23 12K 800 tex carbon fibers, manufactured by Teijin Carbon, are utilized in the process. Each spool is mounted on an electronically controlled unwinding unit provided by Texmar, which ensures precise fiber tension during unwinding. The carbon fibers are impregnated using a roller impregnation technique with an epoxy resin composed of Araldite LY 1564 (epoxy) and Aradur 3486 (hardener) from Huntsman, in a ratio of 100:34. The resin bath temperature is kept at 45°C.

Alternate image: Figure 5. Setup of the experiment. ...

Figure 5. Setup of the experiment.

In this experiment, two different patterns are wound around the mandrel. The first pattern is a hoop winding, where the delivery eye moves from one side to the other, depositing a single layer of fiber material onto the mandrel. The second pattern is a helical winding, executed at an angle of +-70°, resulting in two layers of fiber material.

During the winding process, the incoming fiber tape is observed to be moving away from the image center of the camera, as shown in Fig. 6. The horizontal distance at which the tape moves away from the image center increases as the winding angle (φ) decreases. Thus, the vertical distance between the camera and the mandrel is adjusted to ensure that the incoming tape remains visible at all times throughout the winding process for a winding angle of up to 70°.

Alternate image: Figure 6. Illustration of the tape lagging behind the position of image center ...

Figure 6. Illustration of the tape lagging behind the position of image center

The horizontal distance (d) of the mandrel section overlooked by the camera is measured at 225 mm, as shown in Fig. 6. Since this distance corresponds to an image width (N) of 640 pixels, the conversion factor (px to mm) can be calculated as follows:

undefined

As mentioned earlier, the smaller the winding angle, the further away the camera must be from the mandrel, resulting in an increased conversion factor which, in turn, reduces the potential accuracy in calculating the tape’s width and position. This issue will be further addressed in the final section of this paper.

Note: Distortion errors of the camera lens, which may cause the actual conversion factor (c) to vary across pixels, as well as the decreasing distance (d) with an increasing number of material layers are outside the scope of this work.

The software parameters are intentionally set to define the tape width as slightly thinner than what is observed in practice to induce overlaps in the actual winding pattern. Throughout the winding process, the IR-images, as well as the linear position (y) of the Y-Axis and the angular position (α) of the C-Axis, are recorded, as presented in Figs. 7 and 8.

Alternate image: Figure 7. Recorded axis data during hoop winding. ...

Figure 7. Recorded axis data during hoop winding.

Alternate image: Figure 8. Recorded axis data during helical winding. ...

Figure 8. Recorded axis data during helical winding.

The software prototype used for recording the machine axis positions and visualizing the winding process, which will be discussed in the following sections, is developed using ‘Processing,’ a free graphical library and integrated development environment (IDE) based on the Java language. For recording machine axis positions, an additional Java library from Beckhoff (TE1000 | TwinCAT 3 ADS DLL Java) is integrated into the software.

 

Tape detection and digital twin

After the winding process, the recorded frames of the IR images and the axis data are loaded into the software prototype, where they are first synchronized. In the next step, an edge detection algorithm is used to calculate the width and position of the tape relative to the image center for each frame. The algorithm starts by extracting the center row of the camera image, referred to as temperature profile (t ⃗), as depicted in Fig. 9. If the temperature profile exhibits relatively strong noise, it can be smoothed by averaging over several neighboring elements if necessary. The value of each pixel or element in the profile array is described by (t_i), where (i) represents the position, or index, of an element in the array, ranging from 0 (left side of the image) to 639 (right side). A gradient (g_i) is then calculated for each position (i) of the temperature profile by considering m neighboring elements on each side and storing the results in a separate array of the same length, known as the gradient profile (g ⃗). To further empathize the amplitude of the gradient value around the tape edges, the gradient value for each position along the gradient profile is weighted with the temperature value at the corresponding position.

undefined

If the contrast between the incoming tape and the previously placed material is sufficient, the edges of the tape can be clearly identified in the gradient profile, as shown in Fig. 9. The positions of the left and right edges of the tape can be determined by searching for the maximum and minimum values in the gradient profile. In order for the algorithm to decide whether or not the contrast is sufficient, a threshold is applied. A maximum in the gradient profile is considered a valid left edge only if it is the sole peak or the first peak (from the left) above the threshold. Conversely, a minimum is considered to be a right edge if it is the only valley or the first valley (from the right) below the threshold. The threshold value is determined based on the standard deviation (s) [7] of the values within the gradient profile. For this algorithm, it has been extended with an additional scaling factor (v=1) which can be adjusted if necessary.

undefined
Alternate image: Figure 9. Visualization of the edge detection algorithm. ...

Figure 9. Visualization of the edge detection algorithm.

After determining the index positions of the left edge (i') and the right edge (i'') the width (w) of the tape in the axial or y-direction is then calculated for each frame (f). This is done by counting the pixels between and including the left and right edges, and then multiplying the sum width by the conversion factor (c = 0.35) from equation (4).

undefined

The offset (o) of the tape center relative to the image center can be calculated accordingly.

undefined

If the contrast between the incoming tape and the previously placed material is insufficient, another approach is needed. During helical winding at higher speeds, for example, when the tape reaches a turning point at the end of the mandrel, the incoming tape crosses another tape section which was placed shortly before. The incoming tape. still relatively warm. can become indistinguishable from the intersecting tape, which impedes the algorithm’s ability to differentiate between their edges. The same issue occurs if there are gaps within the tape. Both scenarios are depicted in Fig. 10.

Alternate image: Figure 10. Example of an indistinct left edge. ...

Figure 10. Example of an indistinct left edge.

In Fig. 10, the right edge is accurately identified, but the left edge cannot be reliably detected because there are multiple peaks above the threshold, with the most prominent peak corresponding to a gap within the tape itself. In this case, the algorithm uses the position of the left edge from the previous frame as starting point and searches for the nearest peak along the gradient profile. It needs to be mentioned that this approach is effective only for temporary disturbances. If the disturbance persists over a longer period, the algorithm will eventually lose track of the edge.

Additionally, to further minimize potential disturbances and increase the algorithm’s speed, the edge detection algorithm can be restricted to a smaller region within the camera image by approximating the tape’s position and reducing the search for edges within close proximity. To approximate the position of the tape, the following equation can be used which is employed by the winding software to calculate the twist angle (τ) of the delivery eye [8].

undefined

The twist angle and the distance (z) between the delivery eye and the mandrel axis can be determined be reading the axis positions of the W-axis and Z-axis (see Fig. 5). By rearranging the equation to the angle (φ), it becomes possible to estimate the position of the tape in the image.

The following simplified flowchart depicts the basic process of the current tape detection algorithm.

Alternate image: Figure 11. Flow chart of the tape detection algorithm. ...

Figure 11. Flow chart of the tape detection algorithm.

For each frame (f), the position of the tape along the mandrel- Y-axis can then be calculated by adding the tape’s offset (o) from the image center (equation (5)) to the position of the camera (y).

undefined

The tape position in circumferential direction (u) of the mandrel can be determined by the rotation angle (α) of the mandrel- or C-axis and the radius of the mandrel.

undefined

For each frame (f), the measured width (w) of the tape in the axial direction can be represented by a line element (horizontal orange line Fig. 12). This line element is positioned at (y') along the mandrel axis and at position (u) along the circumferential direction. By considering the line elements of two consecutive frames, as shown Fig. 12, we can calculate the winding angle (φ).

undefined
Alternate image: Figure 12. Process of visualizing the winding patterns. ...

Figure 12. Process of visualizing the winding patterns.

The actual width of the tape (w') perpendicular to the fiber direction can then be calculated by the width of the tape in axis direction (w) and the winding angle (φ).

undefined

In accordance with the methods outlined in a separate publication, two consecutive line elements are connected to form a quadrangle that represents a tape section [6]. To visualize the winding process, this quadrangle is subsequently drawn on a texture map that represents the lateral surface of the mandrel. This texture map is then wrapped around a 3D-cylinder with identical geometric properties to the mandrel. By rotating the cylinder to the appropriate angle based on the frame and incorporating an additional body to represent the delivery eye, the software can simulate the winding process.

Alternate image: Figure 13. Visualization of the winding process by the software. ...

Figure 13. Visualization of the winding process by the software.

Each pixel of the texture map can be colored differently to provide visual feedback regarding information such as the winding angle or the number of material layers at that pixel. To calculate the number of layers at each pixel of the texture map, the software counts how many times each pixel has been within the region of an added quadrangle.

 

Result

Consequently, a three-dimensional depiction of the mandrel is achieved, accompanied by a texture map that illustrates the tape’s path across the mandrel’s surface. This pattern can be color-coded based on the winding angles or the number of layers present at each point on the texture map. The latter aspect holds significant importance in identifying and localizing gaps and overlaps within the laminate structure. Fig. 14 illustrates the first trial of winding a circumferential pattern. The goal is to cover the mandrel with a single layer of material. Regions displaying two or more layers indicate an overlap (yellow), while areas lacking any layer signify a gap (grey).

Alternate image: Figure 14. Hoop winding; winding angle (top), number of layers (bottom). ...

Figure 14. Hoop winding; winding angle (top), number of layers (bottom).

In the context of the second trial, where a helical pattern is applied, it is anticipated that there will be two material layers. Consequently, overlaps are represented by a minimum of three layers, while gaps are indicated by fewer than two layers, as illustrated in Fig. 15.

Alternate image: Figure 15. Helical winding (70°); winding angle (top), number of layers (botto ...

Figure 15. Helical winding (70°); winding angle (top), number of layers (bottom).

By counting the connected elements of the texture map that represent a gap or an overlap, further information on the size of the gaps and overlaps can be quantified.

 

Conclusion and outlook

The findings of this study demonstrate that the utilization of an infrared camera effectively captures the winding patterns of both circumferential and helical windings within the cylindrical section of a mandrel. Furthermore, the captured patterns can be converted into a digital twin for further analysis, including the visualization of gaps and overlaps in the laminate structure.

However, it has been shown that the location at which the tape first contacts the mandrel during the winding process is situated behind the position of the delivery eye (see Fig. 6). As the winding angle decreases, the distance between the delivery eye and the tape contact point gradually increases. Consequently, the camera must be positioned further away to capture a larger area, which reduces the number of pixels along the tape width and therefore decreases measurement accuracy. To address this issue, the camera needs to be moved closer to the mandrel. Two different methods will be tested in the future. The first method involves utilizing multiple cameras positioned next to each other to cover a larger area. By mounting each camera closer to the mandrel, the captured images can later be stitched together, resulting in higher resolution along the mandrel axis. The second approach entails attaching the IR-camera to an additional linear axis. By reading the W-axis and Z-axis of the winding machine (see Fig. 5) during the winding process, the tape’s approximate position can be determined using equation (6), which is used by the winding software to calculate the twist angle of the delivery eye. Consequently, the camera can be relocated to the estimated position of the tape, allowing for closer proximity to the mandrel.

To further investigate how imperfections impact the strength and rigidity of the component, plans are in place to transfer the winding patterns to a finite element model (FEM).

References:

1.
Leichtbaustrategie der Bundesregierun. BMWK - Bundesministerium für Wirtschaft und Klimaschutz. July 2023. Accessed 8.09.2023. https://www.bmwk.de/
2.
Azeem M, Ya HH, Alam MA i in. Application of Filament Winding Technology in Composite Pressure Vessels and Challenges: A Review. J Energy Storage. 2022;49:103468. doi:10.1016/j.est.2021.103468
3.
Regulation No 134 of the Economic Commission for Europe of the United Nations (UN/ECE) — Uniform provisions concerning the approval of motor vehicles and their components with regard to the safety-related performance of hydrogen-fuelled vehicles (HFCV) [2019/795]. Official Journal of the European Union; May 2019.
4.
Hopmann C, Magura N, Rozo Lopez N, Schneider D, Fischer K. Detection and evaluation of the fibers' deposition parameters during wet filament winding. Polym Eng Amp Sci. 2021;61(5):1353-1367. doi:10.1002/pen.25649.
5.
Hopmann C, Magura N, Müller R, Schneider D, Fischer K. Impact of winding parameters on the fiber bandwidth in the cylindrical area of a hydrogen pressure vessel for generating a digital twin. Polym Compos. 2022;43(3):1577-1589. doi:10.1002/pc.26479.
6.
Rozo Lopez N, Tao Y, Çelik H, Hopmann C. Development of an image processing algorithm ( IPA‐Delfin ) for the digital reconstruction of composite overwrapped pressure vessels. Polym Compos. 2023. doi:10.1002/pc.27253.
7.
Sekander Hayat Khan M. Standard Deviation. In: International Encyclopedia of Statistical Science. Springer Berlin Heidelberg; 2011:1378-1379. doi:10.1007/978-3-642-04898-2_535.
8.
Vasiliev VV. Composite pressure vessels: Analysis, design, and manufacturing. Bull Ridge Pub.; 2009.
9.
Rousseau J, Perreux D, Verdière N. The influence of winding patterns on the damage behaviour of filament-wound pipes. Compos Sci Technol. 1999;59(9):1439-1449. doi:10.1016/s0266-3538(98)00184-5.
10.
Cohen D. Influence of filament winding parameters on composite vessel quality and strength. CompositesA. 1997;28(12):1035-1047. doi:10.1016/s1359-835x(97)00073-0